Tombstoning, cold joints or batch defects appear after SMT reflow. Why?
Conclusion: check the pads, the stencil and the reflow profile first, then whether the parts have absorbed moisture (MSL).
Symptoms
After reflow some components are shifted or tombstoned, or there is no electrical connection and cold joints appear across a whole batch.
Common causes
- The pad design does not match the recommended land pattern in the datasheet
- Uneven heating of the two pads, or asymmetric stencil apertures
- The parts have absorbed moisture (MSL exceeded), so internal vapour expands during reflow and causes the popcorn effect
- Storage humidity is too high, or the parts were not used within the specified time after the bag was opened
Recommended actions
- Redesign the pads and stencil apertures according to the land pattern in the datasheet
- Check the reflow profile (preheat, soak, peak temperature and time above liquidus)
- Confirm the MSL level and, if it is exceeded, bake according to J-STD-033 (for example 125 C for 24 h)
- Record the time since the bag was opened, and bake again or store in a dry cabinet once the floor life is exceeded